Log end sealers and sealing slabs: what FPL and FPInnovations publish
A 2024 Forest Products Laboratory trial found three end coatings cut end checks on red oak boards over a year of air-drying, with no difference among them. FPInnovations tested five coatings on maple and birch logs.
Checked against the sources at the bottom of this page on October 21, 2026. Rules, fees and pay change: the source has the last word.
One Forest Products Laboratory (FPL) research paper, two editions of the FPL Wood Handbook and one FPInnovations report cover end coatings on logs and lumber. None of them tests sealing the faces of slabs, so that part of the subject has no figure.
Why ends check
FPL Research Paper RP-722 (Lyon, Buntrock, Wiemann and Bowe, 2024) explains the mechanism. Lumber dries from the surface inward, so surface cells shrink first and drying stress builds, and the ends dry fastest. Moisture moves 10 to 15 times faster along the grain than across it. The paper reports that the stress begins when lumber is first sawn and lasts until about one-third of the moisture has gone, and that all surface and end checks form in that early stage.
The paper gives one cost figure: a 4 inch end split or check on both ends of an 8 foot piece causes an 8 percent volume loss. FPInnovations calls checking at log and lumber ends one of the most common defects, often a great loss of wood value.
What the Wood Handbook prints
Both editions of the Wood Handbook carry a sentence on end coatings in the drying chapter. The 2021 edition has a further one in the decay chapter.
| Edition | Statement on end coatings |
|---|---|
| FPL-GTR-190 (2010), chapter 13 | End coatings, on either the log or freshly sawn (green) lumber, are an effective preventative measure against end fracturing. |
| FPL-GTR-282 (2021), chapter 13 | Air drying can bring end splitting, and end coating may alleviate end checking. End coatings on logs or freshly sawn green lumber are called an effective preventative measure. |
| FPL-GTR-282 (2021), chapter 14 | For log storage longer than 2 to 3 months, an end coating is needed to prevent seasoning checks, through which infection can enter the log. |
The chapter 14 sentence sits in the passage on protecting logs from fungal damage. It says preservative sprays protect most timber species for 2 to 3 months, except in severe decay hazard climates, and that rapid conversion or storage in water is the surest way to avoid fungal damage.
The 2024 FPL air-drying trial
The trial used 59 red oak boards, No. 1 Common grade, sawn in July 2021 and air-dried for 12 months near Antigo, Wisconsin, to an average moisture content of 11.8 percent. Of the 56 boards used for the comparison, 42 were coated on both ends and 14 were left as controls. Three coating types were tested: exterior latex paint, an emulsified wax and a roofing compound.
| Treatment | Ends with no defect | Ends with a defect | Longest defect class |
|---|---|---|---|
| Latex paint (27 ends) | 25 | 2 | 1 to 2 inches |
| Emulsified wax (29 ends) | 23 | 6 | 1 to 2 inches |
| Roofing compound (28 ends) | 19 | 9 | Over 2 inches (3 ends) |
| Uncoated (28 ends) | 1 | 27 | Over 2 inches (9 ends) |
The analysis found every coating different from the uncoated control and no significant difference among the three coatings. The authors suggest the black roofing compound may have absorbed heat and that, being oil-based, it may not have stuck to wet end grain. They add that most boards with it still showed no defects. Latex paint and wax were easy to apply and clean up, and the roofing compound was the most difficult and messy.
The paper also records how mills and small producers coat ends. It reports that large lumber makers use a commercial emulsified wax applied by brush, roller or spray, and that small producers have used exterior latex paint, roofing compound and their own recipes. Historic coatings it lists are white lead, synthetic resin, wax, asphalt, pitch, paraffin and paint. It states the sawmill industry has coated ends for more than 100 years.
The FPInnovations test on logs and boards
FPInnovations report 5366 (Yang and Normand, March 2008, 39 pages) tested five commercial coatings from Canada and the United States on sugar maple and yellow birch. It used 120 fresh logs, 200 boards and 100 components per species in 2006 and 140 logs per species in 2007, with two application methods. All five products reduced check development in logs, lumber and components. The best treatment cut checking in lumber and components by up to 100 percent, and in logs by up to 80 percent over 8 weeks.
Effectiveness varied with species, product type, treating time, application method and storage conditions, and no product was superior under every test condition. The report adds that coating effectiveness on different species is not well established, and that the expected result is often not reached.
What is not printed
None of these sources gives a drying-time benefit, a coating thickness in millimetres, or a result for sealed slabs or for species other than red oak, sugar maple and yellow birch. For the wider drying subject, see the guide to wood moisture and drying and the guide to log storage before milling.
Sources
- USDA Forest Service Forest Products Laboratory, Effects of end coatings on defects during air-drying of lumber (FPL-RP-722, Lyon et al., December 2024), read October 21, 2026
- USDA Forest Service Forest Products Laboratory, Wood handbook: Wood as an engineering material (FPL-GTR-282, Ross, 2021), chapters 13 and 14, read October 21, 2026
- USDA Forest Service Forest Products Laboratory, Wood handbook: wood as an engineering material (FPL-GTR-190, Ross, 2010), chapter 13, read October 21, 2026
- FPInnovations Research Library, End coating to prevent checks on hardwood (Yang and Normand, report 5366, March 2008), read October 21, 2026