Moisture targets by end use: what the Wood Handbook, GOV.UK and Oregon State print for lumber, furniture and fuel
The Wood Handbook prints an 8 percent average for interior wood in most US areas and 12 percent for exterior wood. GOV.UK sets 20 percent or less for Ready to Burn firewood in England.
Checked against the sources at the bottom of this page on October 15, 2026. Rules, fees and pay change: the source has the last word.
This page reports what the official source says. It is not legal advice: ask the office named here.
The US Forest Service Forest Products Laboratory publishes the Wood Handbook as General Technical Report FPL-GTR-282. Chapter 13, by Richard Bergman, ties each target to the moisture content the wood meets in service. Wood installed at that level shrinks and swells less afterward, and the chapter names floor buckling and cracked furniture as the problems.
Targets printed in each source
| End use | Printed figure | Source |
|---|---|---|
| Interior woodwork, flooring, furniture and wood trim, most areas of the United States | 8 percent average, individual pieces 6 to 10 percent | Wood Handbook, Table 13-2 |
| Interior woodwork, flooring, furniture and wood trim, dry southwestern area | 6 percent average, individual pieces 4 to 9 percent | Wood Handbook, Table 13-2 |
| Interior woodwork, flooring, furniture and wood trim, damp warm coastal area | 11 percent average, individual pieces 8 to 13 percent | Wood Handbook, Table 13-2 |
| Exterior siding, wood trim, sheathing and laminated timbers, most areas | 12 percent average, individual pieces 9 to 14 percent | Wood Handbook, Table 13-2 |
| Exterior siding, wood trim, sheathing and laminated timbers, dry southwestern area | 9 percent average, individual pieces 7 to 12 percent | Wood Handbook, Table 13-2 |
| Exterior siding, wood trim, sheathing and laminated timbers, damp warm coastal area | 12 percent average, individual pieces 9 to 14 percent | Wood Handbook, Table 13-2 |
| Dry softwood lumber | Maximum 19 percent in the American Softwood Lumber Standard. Grade mark KD 15 usually has a maximum of 15 percent | Wood Handbook, chapter 13 |
| Lumber air-dried outdoors under cover | About 12 to 14 percent in Western Oregon and 8 to 10 percent in Eastern Oregon | Oregon State Extension, EM 8612 |
| Firewood and wood briquettes sold in England in volumes under 2 cubic metres | 20 percent or less, certified as Ready to Burn | GOV.UK, Defra guidance |
| Slabs, tabletops and other single products | No value printed beyond the interior and exterior rows above | None of the three |
Interior and exterior wood in the Wood Handbook
The Wood Handbook splits the United States into three areas in its Figure 13-1. Most of the country has an interior average of 8 percent. The dry southwest sits at 6 percent and the damp, warm coastal area at 11 percent. Exterior wood depends mainly on outdoor conditions, and the chapter lists monthly outdoor equilibrium moisture content for many US cities in Table 13-1.
The chapter holds interior wood to tighter limits than outdoor wood. A lot is probably satisfactory when the average falls within 1 percent of the recommended figure and every piece sits inside the individual limits.
Commercial practice in the Handbook kiln-dries flooring and furniture stock slightly below the service moisture content. This anticipates a moderate rise during processing, transport and construction. Common grades of softwood boards and dimension lumber are not normally dried to the Table 13-2 values.
Lumber dried outdoors in the Oregon State publication
Oregon State Extension's EM 8612 says drying wood to the average moisture content of its end use keeps shrinking and swelling to a minimum. Strength properties rise as wood dries below the fiber saturation point, which the publication puts at about 25 to 30 percent.
Air-drying takes several months to almost a year, depending on conditions, species and size. Wood stored outdoors under cover reaches about 12 to 14 percent in Western Oregon and 8 to 10 percent in Eastern Oregon. Lumber air-dried properly through the summer in western Oregon should reach 12 to 14 percent by fall. The Wood Handbook gives extremes for air-drying 25 mm (1 inch) lumber to 20 to 25 percent. Low-density species such as pine and spruce take 15 to 30 days in favorable places and seasons. Oak and birch take 200 to 300 days in northern locations at unfavorable times.
Fuel in the GOV.UK guidance
GOV.UK's guidance on selling wood for domestic use in England covers firewood in single retail bags and loose bulk deliveries under 2 cubic metres. These can be supplied or sold only if certified as Ready to Burn, which confirms a moisture content of 20 percent or less. Certification lasts 12 months. Sales of 2 cubic metres or more need no certification, but the supplier must hand the customer a notice on how to dry, store and check the moisture of the wood.
Local authorities enforce the rules. Wood stored above 20 percent moisture, or sold without the logo or correct labelling, can bring a £300 fixed penalty from the local authority. The courts can set a larger fine depending on the severity of the offence.
Gaps in the printed targets
The GOV.UK figure is a legal limit for sold fuel, and the Wood Handbook figures are installation targets for products. Neither source prints a firewood target for use in a particular stove, and the Wood Handbook table has no fuel row.
Sources
- US Forest Service, Forest Products Laboratory, Wood Handbook, General Technical Report FPL-GTR-282, chapter 13, Drying and Control of Moisture Content and Dimensional Changes, read October 15, 2026
- GOV.UK, Defra, Selling wood for domestic use in England (last updated July 7, 2022), read October 15, 2026
- Oregon State University Extension, EM 8612, Air and Shed Drying Lumber, read October 15, 2026