Air-drying lumber: drying times, sticker spacing and moisture targets from FPL and extension
The Forest Products Laboratory puts air-drying 1-inch lumber at 15 to 30 days for pine and 200 to 300 days for oak and birch. Clemson Extension gives sticker spacing of 12 to 24 inches for 4/4 hardwood.
Checked against the sources at the bottom of this page on October 16, 2026. Rules, fees and pay change: the source has the last word.
The US Forest Products Laboratory (FPL), Oregon State University Extension and Clemson Extension all publish air-drying figures for sawn lumber. None prints one table of drying time by thickness and species group. Each gives its own figures under its own conditions.
What air-drying is
The FPL Wood Handbook, chapter 13, defines air-dry lumber as lumber dried by exposure to the air outdoors or in a shed, or by forced circulation of air not heated above 49 °C (120 °F). It gives the main purpose of air-drying as evaporating as much water as possible before end use or before kiln drying. Air-drying down to 20% to 25% moisture content before the kiln saves energy, because kiln drying uses the most energy of all wood production processes, and it cuts the kiln capacity needed.
OSU Extension publication EM 8612, published September 1995 and reviewed in 2024, says air-drying means stacking lumber and exposing it to the outdoors. The final moisture content depends on air temperature, relative humidity and drying time. It also says air-drying starts as soon as the tree is cut.
Drying time
| Publication | Time printed | Conditions named |
|---|---|---|
| FPL Wood Handbook, ch. 13 | 15 to 30 days for 1-inch lumber of low density species such as pine, spruce, red alder and soft maple | Favorable locations and times of year; target 20% to 25% moisture content |
| FPL Wood Handbook, ch. 13 | 200 to 300 days for 1-inch lumber of slow-drying species such as sinker hemlock and pine, oak and birch | Northern locations, stacked at unfavorable times of year |
| OSU Extension EM 8612 | Several months to almost a year | Depends on outside conditions and on lumber species and size |
| OSU Extension EM 8612 | Two-inch lumber can take three to four times as long as 1-inch lumber of the same species | Same species, same target moisture content |
| Clemson Extension | About one year for every inch of board thickness to reach equilibrium moisture content | General rule often mentioned by experienced sawyers, as Clemson reports it |
The three publications are not measuring the same thing. FPL gives the extremes at a 20% to 25% target. OSU gives a range for Oregon. Clemson gives a rule per inch of thickness for drying all the way to equilibrium. The FPL chapter adds that the time varies widely with species, thickness, location and the time of year the lumber is stacked.
Moisture contents the pages print
- FPL: commercial air-dry stock usually has a moisture content of 20% to 25% for dense hardwoods and 15% to 20% for softwoods and low-density hardwoods.
- FPL: softwood framing lumber is usually dried to an average of 15%, not to exceed 19%. Appearance grades are dried to 10% to 12%, and furniture, cabinet and millwork stock to 7% to 9%. Hardwood for furniture, flooring, cabinets and millwork is usually dried to 6% to 8%.
- OSU: wood stored outdoors and under cover dries to about 12% to 14% in western Oregon and 8% to 10% in eastern Oregon. Lumber air-dried through the summer in western Oregon should reach 12% to 14% by fall.
- Clemson: freshly cut lumber has a moisture content that can vary from 30% to over 100%, and the equilibrium moisture content in South Carolina varies from 11.6% to 14.5%.
Stickers and spacing
OSU says one-inch thick stickers are commonly used for air-drying, that they should be dry and of uniform size, and that they should be wider than they are thick. Ideally a bottom support bunk sits under every row of stickers, and stickers align one above the other. OSU puts a sticker distance of about 18 to 24 inches as sufficient for lumber of almost any size, and says some hardwoods, such as elm, call for stickers every 12 inches. Thicker lumber needs less support, so its stickers can sit farther apart.
Clemson gives stickers a typical length of 3 to 4 feet and a cross-section of about three-quarters of an inch by one inch. For hardwood 4/4 lumber it puts spacing at 12 to 24 inches. For lumber 8/4 (2 inches) or thicker it puts spacing at less than 48 inches. For lumber cut on a portable sawmill, it says a spacing of 16 to 24 inches is usually adequate.
The OSU and Clemson ranges overlap at 18 to 24 inches. Neither page says anything different for slabs than for boards, and neither prints sticker figures by species group other than the elm exception.
End checking and drying rate
FPL lists the limits of air-drying. The rate is very slow in cold winter months. Hot dry winds can increase surface checking and end splitting. Warm humid periods with little air movement can encourage fungal stain. Carrying a large inventory of high-value lumber for long periods costs money. End coating may reduce end checking and splitting.
OSU describes end checks as forming because moisture moves much faster through the ends of a board than through its sides, so the ends dry faster than the middle. For species prone to checking, such as oak, it says an end coating is applied as soon as possible, preferably in the woods before the logs are hauled. OSU also reports that lumber stacked over concrete or asphalt dries faster than lumber over bare or vegetation-covered ground. Its stack roof extends 2 to 3 inches past the lumber on all sides. East of the Cascades lumber can air-dry too fast: 90 F and 15% relative humidity gives an equilibrium moisture content below 4%.
OSU Table 1 prints maximum safe daily rates of moisture loss for 4/4 hardwood lumber.
| Species | Maximum daily moisture loss |
|---|---|
| Soft maple | 13.8% |
| American elm | 10.4% |
| Walnut | 8.2% |
| Hard maple | 6.5% |
| Yellow birch | 6.1% |
| Cherry | 5.8% |
| Eastern red oak | 3.8% |
| Eastern white oak | 2.5% |
| Oregon white oak | 2.0% (estimated) |
OSU marks the eastern figures as empirical rates from Wengert, 1980, and the western ones as estimates based on anatomical similarities. OSU says some hardwoods, especially oaks, have low maximums of about 1% to 2% per day, and that these are maximum per-day values, not averages over longer periods.
Air-drying before the kiln
OSU says green 4/4 white oak can take more than a month to kiln-dry, while air-dried 4/4 white oak can be kiln-dried in one to two weeks. Clemson says commercial kilns can often dry a batch in two to eight weeks, and solar kilns take six weeks to several months. Kiln types are in kilns for firewood and lumber, and moisture basics are in wood moisture and drying.
Sources
- USDA Forest Service, Forest Products Laboratory, Wood Handbook chapter 13 Drying and Control of Moisture Content and Dimensional Changes, FPL-GTR-282, read October 16, 2026
- Oregon State University Extension, Air- and shed-drying lumber, EM 8612, published September 1995, reviewed 2024, read October 16, 2026
- Clemson University Extension, Using your portable sawmill to cut stickers for lumber drying, read October 16, 2026